<rss 
	version="2.0"
	xmlns:content="http://purl.org/rss/1.0/modules/content/"
	xmlns:dc="http://purl.org/dc/elements/1.1/" 
	xmlns:atom="http://www.w3.org/2005/Atom"
	xmlns:media="http://search.yahoo.com/mrss/"
>

<channel>
	<atom:link href="https://thenarwhal.ca/feed/" rel="self" type="application/rss+xml" />
	<title>The Narwhal | News on Climate Change, Environmental Issues in Canada</title>
	<link>https://thenarwhal.ca</link>
  <description>The Narwhal’s team of investigative journalists dives deep to tell stories about the natural world in Canada you can’t find anywhere else.</description>
  <language>en-US</language>
  <copyright>Copyright 2026 The Narwhal News Society</copyright>
	<lastBuildDate>Tue, 10 Nov 2026 23:01:24 +0000</lastBuildDate>
	<image>
		<title>The Narwhal | News on Climate Change, Environmental Issues in Canada</title>
		<url>https://thenarwhal.ca/wp-content/uploads/2026/03/the-narwhal-rss-icon.png</url>
		<link>https://thenarwhal.ca</link>
		<width>144</width>
		<height>144</height>
	</image>
	    <item>
      <title>Pipeline Expert: Over 90% Probability of Line 9 Rupture with Tar Sands Dilbit</title>
      <link>https://thenarwhal.ca/pipeline-expert-90-percent-probability-line-9-rupture-dilbit/?utm_source=rss</link>
			<guid isPermaLink="false">http://localhost.com/narwhal/2013/10/22/pipeline-expert-90-percent-probability-line-9-rupture-dilbit/</guid>
			<pubDate>Tue, 22 Oct 2013 21:19:28 +0000</pubDate>			
			<description><![CDATA[The international pipeline safety expert who last August described Enbridge&#8217;s Line 9 pipeline as &#8220;high risk for a rupture&#8221; now says the probability of Line 9 rupturing is &#8220;over 90%.&#8221; &#8220;I do not make the statement &#8216;high risk for a rupture&#8217; lightly or often. There are serious problems with Line 9 that need to be...]]></description>
			<content:encoded><![CDATA[<figure><img width="300" height="233" src="https://thenarwhal.ca/wp-content/uploads/2018/04/pipelinespillmayflowerarkansas2-300x233.jpg" class="attachment-banner size-banner wp-post-image" alt="" decoding="async" fetchpriority="high" srcset="https://thenarwhal.ca/wp-content/uploads/2018/04/pipelinespillmayflowerarkansas2-300x233.jpg 300w, https://thenarwhal.ca/wp-content/uploads/2018/04/pipelinespillmayflowerarkansas2-300x233-20x16.jpg 20w" sizes="(max-width: 300px) 100vw, 300px" /><figcaption><small><em></em></small></figcaption></figure> <p>The international pipeline safety expert who last August described Enbridge&rsquo;s Line 9 pipeline as <a href="https://thenarwhal.ca/2013/08/14/line-9-pipeline-high-risk-rupture-says-pipeline-expert">&ldquo;high risk for a rupture&rdquo;</a> now says the probability of Line 9 rupturing is &ldquo;over 90%.&rdquo;</p>
<p>&ldquo;I do not make the statement &lsquo;high risk for a rupture&rsquo; lightly or often. There are serious problems with Line 9 that need to be addressed,&rdquo; Richard Kuprewicz, a pipeline safety expert with over forty years of experience in the energy sector, said in an interview with DeSmog Canada.</p>
<p><a href="http://www.citynews.ca/2013/10/19/hundreds-protest-enbridges-line-9-pipeline/" rel="noopener">Hundreds rallied in Toronto on the weekend</a> to voice their opposition to Enbridge&rsquo;s plans to ship Alberta tar sands bitumen from Sarnia to Montreal through the 37-year-old Line 9 pipeline.</p>
<p>Kuprewicz also expressed concerns about transporting diluted bitumen through Line 9 saying it will increase the growth rates of cracks on the pipeline. Line 9 lies in the most populated part of Canada and crosses the St. Lawrence River and major waterways flowing into Lake Erie and Lake Ontario. A Line 9 spill could pollute the drinking water of millions of Canadians. &nbsp;</p>
<p><!--break--></p>
<p><img alt="" src="https://thenarwhal.ca/wp-content/uploads/files/Map%20-%20Line%209.png"></p>
<p><strong>Extensive Stress Corrosion Cracking on Line 9</strong></p>
<p>&ldquo;Existing SCC (stress corrosion cracking) on Line 9 can worsen due to the increase in pressure cycling associated with shipping dilbit (diluted bitumen). This could lead to a rupture,&rdquo; explains Kuprewicz.</p>
<p>The thick heavy crude&nbsp;<a href="http://www.api.org/~/media/Files/Oil-and-Natural-Gas/Oil_Sands/Diluted-Bitumen.pdf" rel="noopener">bitumen is diluted with a condensate</a> (natural gas or naphtha) so it can flow through pipelines. &lsquo;<a href="http://insideclimatenews.org/news/20130909/dilbit-exxons-pegasus-may-have-contributed-pipelines-rupture" rel="noopener">Pressure cycling</a>,&rsquo;&nbsp;or the variations in operating pressures of a pipeline, increase with dilbit, because dilbit can vary more in composition than light conventional oil. The greater swings in the levels of operating pressures can create cracks in a pipeline.</p>
<p>Kuprewicz examined Enbridge&rsquo;s assessments of Line 9 and <a href="https://www.neb-one.gc.ca/ll-eng/livelink.exe/fetch/2000/90464/90552/92263/790736/890819/956564/956632/981386/A3J7T4_-_Attachment_B-_ACCUFACTS_PIPELINE_SAFETY_REPORT.2013.08.05?nodeid=981150&amp;vernum=0&amp;redirect=3" rel="noopener">found evidence of extensive stress corrosion cracking on Line 9</a>, most likely caused by the pipeline&rsquo;s external protective coating (polyethylene tape or PE-tape) separating from the sections of Line 9, allowing water to damage the pipe.</p>
<p>Kuprewicz has seen this problem before. He researched the US federal investigation into the Kalamazoo, Michigan dilbit spill &ndash; the largest onshore oil spill in US history &ndash; on behalf of various concerned parties. The disbondment of PE-tape on Enbridge&rsquo;s Line 6B pipeline and subsequent SCC on the pipe caused the rupture. Three million litres of dilbit were spilled into the Kalamazoo River and the surrounding waterways, and the <a href="https://thenarwhal.ca/2013/08/26/official-price-enbridge-kalamazoo-spill-whopping-1-039-000-000">$1 billion cleanup</a> continues to this day.&nbsp;</p>
<p><img alt="" src="https://thenarwhal.ca/wp-content/uploads/files/Line%209%20Rally.jpg"></p>
<p><em>No Line 9 rally in Toronto on October 19th.</em></p>
<p>Enbridge claims that its in-line inspection tool can detect any serious SCC threats to the pipeline. According to Kuprewicz, the in-line detection technology Enbridge is using has yet to be proven effective.</p>
<p><strong>Hydrostatic Testing of Pipelines is the &ldquo;Gold Standard&rdquo; for Safety</strong></p>
<p>&ldquo;Enbridge needs to conduct a hydrostatic test on Line 9. It is the gold standard for pipeline integrity and safety. Canada has a well-established history of hydrotesting its pipelines,&rdquo; Kuprewicz told DeSmog Canada.&nbsp;&nbsp;&nbsp;</p>
<p>A hydrostatic test would pump water through Line 9 at similar pressures to those the pipeline is expected to operate at, but there is no indication that Enbridge plans to conduct hydrostatic testing.</p>
<p>Kuprewicz also questions Enbridge&rsquo;s claims of <a href="http://business.financialpost.com/2013/10/07/enbridge-to-argue-for-reversal-of-pipeline-running-through-ontario-quebec/?__lsa=3c6c-400e" rel="noopener">an automatic shutdown</a> in the event of a pressure drop in Line 9 or a 10-minute shutdown if an unexplained reading comes in from the pipeline. When a pipeline ruptures, pressure loss as well as detecting the drop can take quite a while. The 10-minute shutdown procedure existed at the time of the Kalamazoo spill and it still took Enbridge 17 hours to shut down the ruptured pipeline.</p>
<p>&ldquo;I am not trying to be hard on Enbridge. There are definite improvements they could make to their pipeline management system that would significantly reduce the chances of a Line 9 rupture,&rdquo; says Kuprewicz.</p>
<p><strong>Enbridge Lacks Adequate Liability Insurance for a Line 9 Spill</strong></p>
<p><a href="http://www.thegoodman.com" rel="noopener">The Goodman Group Ltd</a> found that, in the event of a Line 9 spill, Enbridge&rsquo;s US$685 million liability insurance for all its operations (not just Line 9) would be inadequate. The California-based consulting firm says <a href="https://www.neb-one.gc.ca/ll-fre/livelink.exe/fetch/2000/72399/72487/74088/660700/750773/794638/794847/813450/C13-6-11_-_Attachment_E-_TGG_Evidence_NEB_Line_9B_20130806_-_A3J7U2.pdf?nodeid=813481&amp;vernum=0&amp;redirect=3&amp;redirect=4" rel="noopener">Enbridge needs $3 billion of liability insurance for Line 9</a> alone.</p>
<p>"This is especially true in Toronto and Montreal, where the pipeline runs parallel to or across key urban infrastructure and could threaten the drinking water supply, resulting in multi-billion dollar costs," warned Ian Goodman, president of the Goodman Group.</p>
<p><img alt="" src="https://thenarwhal.ca/wp-content/uploads/files/Line%209%20rally%204.jpg"></p>
<p><em>No Line 9 rally in Toronto on October 19th.</em></p>
<p>Cleanup costs of other onshore oil spills such as Lac-Megantic in Quebec and the Kalamazoo spill were analyzed by the Goodman Group, and Line 9&rsquo;s location in a highly populated area was considered. The firm concluded that a bad Line 9 spill would cost at least $1 billion. The worst-case scenario was pegged between $5-10 billion.</p>
<p><strong>Ontario Demands Independent Third-Party Assessment of Line 9</strong></p>
<p>The Ontario government in some ways echoed the recommendations of Kuprewicz and the Goodman&nbsp;Group on October 17th during a National Energy Board (NEB) public hearing in Toronto.</p>
<p>	Ontario demanded that Enbridge conduct a hydrostatic test on Line 9, and that the company maintain US$1 billion in insurance for the pipeline. The province also called on the NEB to initiate <a href="http://www.thestar.com/news/gta/torontopipeline/2013/10/17/enbridge_ontario_pipeline_plan_continues_to_draw_criticism.html" rel="noopener">an independent third party assessment on the state of Line 9</a>, and not rely solely on Enbridge&rsquo;s findings.</p>
<p>&ldquo;Given the age of the pipeline, its location in a large part of southern Ontario, its additional service life of 30 years or more, and the potential adverse consequences of a rupture, it seems a matter of simple prudence and common sense to ensure the (assessments) are as thorough, comprehensive and as accurate as possible,&rdquo; Rick Jennings, an assistant deputy minister with Ontario&rsquo;s Ministry of Energy told the NEB panel.</p>
<p>&ldquo;In our view, an independent third-party review is required for that assurance,&rdquo; said Jennings.</p>
<p><img alt="" src="https://thenarwhal.ca/wp-content/uploads/files/Line%209%20rally%203.jpg"></p>
<p><em>No Line 9 rally in Toronto on October 19th.</em></p>
<p>The NEB hearings on Line 9 were scheduled to wrap up in Toronto on October 19th, but the NEB postponed the final hearing to an unknown date and location. The NEB could make its final decision on Line 9 as early as January 2014.</p>
<p>Enbridge has applied with the NEB to increase the capacity of Line 9 from 240,000 to 300,000 barrels per day (bpd), reverse the pipeline to flow west-to-east and ship &lsquo;heavy crudes&rsquo; such as dilbit through the line.</p>
<p>Critics of the Line 9 project say the pipeline should not be approved to ship dilbit because of the likelihood of a rupture and the adverse impacts that further expansion of the tar sands will have on climate change and the people and environment of northern Alberta.&nbsp;</p>
<p><em>Image Credit: NWF, Mike Chong, Katheleen Quinn, Mike Eh-En</em></p>

<p><em><strong>The Narwhal’s reporters are telling environment stories you won’t read about anywhere else. Stay in the loop by <a href="https://thenarwhal.ca/newsletter/?utm_source=rss">signing up for our free weekly dose of independent journalism</a>.</strong></em></p>]]></content:encoded>
      <dc:creator><![CDATA[Derek Leahy]]></dc:creator>
						<category domain="post_tag"><![CDATA[bitumen]]></category><category domain="post_tag"><![CDATA[crude oil]]></category><category domain="post_tag"><![CDATA[dilbit]]></category><category domain="post_tag"><![CDATA[Enbridge]]></category><category domain="post_tag"><![CDATA[Enbridge Line 9]]></category><category domain="post_tag"><![CDATA[Kalamazoo Spill]]></category><category domain="post_tag"><![CDATA[National Energy Board (NEB)]]></category><category domain="post_tag"><![CDATA[oil spills]]></category><category domain="post_tag"><![CDATA[pipeline safety expert]]></category><category domain="post_tag"><![CDATA[pipelines]]></category><category domain="post_tag"><![CDATA[Richard Kuprewicz]]></category><category domain="post_tag"><![CDATA[stress corrosion cracking]]></category><category domain="post_tag"><![CDATA[tar sands]]></category><category domain="post_tag"><![CDATA[The Goodman Group Ltd]]></category>			<media:content url="https://thenarwhal.ca/wp-content/uploads/2018/04/pipelinespillmayflowerarkansas2-300x233-300x233.jpg" fileSize="4096" type="image/jpeg" medium="image" width="300" height="233" /><media:thumbnail url="https://thenarwhal.ca/wp-content/uploads/2018/04/pipelinespillmayflowerarkansas2-300x233-300x233.jpg" width="300" height="233" />    </item>
	</channel>
</rss>